Standar lingkungan EU RoHS 2.0 menta eusi lead(Pb) kirang ti 1000ppm.Based on requirment ieu, KINKOU geus ngembangkeun hiji low-lead C17300 jeung kinerja motong na sarua jeung C17300.Kinkou ogé nyadiakeun lead-free tambaga alloy C17200 .Kinerja motong C17200 ieu ogé alus.
1. Komposisi kimiawi kalungguhan low C17300
Modél | Be | Ni+Co | Ni+Co+Fe | Pb | Cu |
C17300 | 1.8-2.0 | ≥0.20 | ≤0.6 | <0.1 | sésa-sésa |
2. Sipat Fisik Jeung Mékanis tinakalungguhan lowC17300
Nagara | perlakuan panas (℃) | Diameter (mm) | Kakuatan Tensile (MPa) | Kakuatan ngahasilkeun (MPa) | Elongation 4xD(%) | Teu karasa | Konduktivitas listrik (IACS,%) | |
HV0.5 | HRB atanapi HRC | |||||||
TB00 | 775 ℃ ~ 800 ℃ | Sadayana | 410-590 | > 140 | > 20 | 159-162 | B45-B85 | 15-19 |
TD04 | 775 ℃ ~ 800 ℃ Solusi + Tiis Prosés Hardening | 8-20 | 620-860 | > 520 | > 8 | 175-257 | B88-B102 | 15-19 |
0.6-8 | 620-900 | > 520 | > 8 | 175-260 | B88-B103 | |||
TH04 | 315 ℃ x 1 ~ 2 jam | 8-20 | 1140-1380 | >930 | > 20 | 345-406 | C27-C44 | 23-28 |
0.6-8 | 1210-1450 | > 1000 | > 4 | 354-415 | C38-C45 |
waktos pos: Jan-12-2021